PTFE البكر

Virgin PTFE (Polytetrafluoroethylene) is the highest purity grade of Teflon, renowned for its near-universal chemical resistance and the lowest coefficient of friction of any solid material. Capable of operating from -200°C to +260°C, it is an essential material for high-performance seals, medical fluidics, and electrical insulators. Jucheng Precision specializes in the precision CNC machining of this exceptionally soft polymer, utilizing ultra-sharp tooling and specialized workholding to overcome challenges like material creep and high thermal expansion. Whether you need complex gas-tight seals or FDA-compliant medical manifolds, our expertise ensures your PTFE parts are delivered with burr-free edges and the precise dimensions required for critical industrial assemblies.

PTFE البكر

أنواع مواد PTFE / التفلون

الدرجة الاسم الشائع الخصائص الرئيسية التطبيقات النموذجية
PTFE البكر الدرجة الكهربائية 99.9% Pure. Lowest friction, highest chemical resistance, and best dielectric properties. FDA compliant. Chemical seals, medical components, laboratory fluidics, electrical insulators.
PTFE ميكانيكي PTFE معاد تصنيعه Contains recycled material. Lower cost but reduced mechanical and electrical properties. Not for food use. الفواصل غير الحرجة، الحلقات، وسادات التآكل.
PTFE المقوى بالزجاج 15% / 25% GF PTFE Reinforced with glass fibers to reduce “cold flow” (creep) and improve compressive strength. Valve seats, gaskets, high-pressure bearings.
PTFE المعزز بالبرونز درجة المحامل Added bronze powder for superior wear resistance and thermal conductivity. Best for heavy loads. Hydraulic cylinder guides, dynamic seals, slider plates.

Virgin PTFE Machining Capabilities

القدرة الوصف الفني ميزة Jucheng
Precision Seal Turning Machining intricate lip profiles and fine grooves for high-performance hydraulic and pneumatic seals. We achieve burr-free edges and Ra 0.4μm finishes directly off the tool, critical for gas-tight and vacuum-tight sealing integrity.
Thin-Wall Sleeve Machining Boring and turning thin-walled PTFE liners and sleeves (down to 0.5mm) without material tearing. Using specialized air-chucks and internal mandrels, we prevent the deformation of the soft PTFE, ensuring perfect concentricity.
Zero-Burr Micro-Drilling Drilling micro-channels in PTFE blocks for laboratory fluidic manifolds and chemical analyzers. Our ultra-sharp micro-tooling ensures internal channels are smooth and free of the stringy burrs common when machining soft Teflon.
Dimensional Stability Control Managing the high thermal expansion of PTFE during the machining process to hold tight tolerances. We machine in a climate-controlled facility and utilize specific “dwell periods” to ensure the part reaches thermal equilibrium before final sizing.

Fabrication Guidelines for Virgin PTFE

حساسية التثبيت:
PTFE is extremely soft and prone to “cold flow” (permanent deformation under pressure). نصيحة: We use custom soft jaws that encapsulate the part or vacuum workholding to prevent clamping marks and geometry distortion.

Thermal Expansion Awareness:
PTFE has a massive coefficient of thermal expansion and undergoes a phase change at 19°C. نصيحة: We maintain a stable 20°C environment for machining and inspection to ensure dimensions remain consistent from our factory to your assembly line.

Sharp Tooling Strategy:
Dull tools will push and smear the material rather than cut it. نصيحة: We use high-rake, polished uncoated carbide tools. This ensures the PTFE is sheared cleanly, resulting in the best possible surface finish and dimensional accuracy.

تخفيف الإجهاد:
Large PTFE billets often contain internal stress from the extrusion process. نصيحة: We perform roughing passes followed by a stabilizing period to allow the material to “relax” before performing final critical finish passes.

التطبيقات الأساسية

Chemical & Fluid Handling
Valve seats, pump diaphragms, and gaskets that require near-universal chemical r

الخصائص

الكثافة 2.14 - 2.18 g/cm³
مقاومة الشد 20 - 35 MPa
معامل الاحتكاك 0.05 - 0.10
الصلابة 55 - 65 Shore D
الاستطالة عند الكسر 250 - 450%
التوصيل الحراري 0.25 واط/م-ك
درجة حرارة الخدمة المستمرة -200 إلى +260 °م
امتصاص الماء < 0.01%
قوة العزل الكهربائي 20 - 60 kV/mm
تقييم قابلية التشغيل متوسط
أقصى حجم للقطعة 2000 × 800 × 600 مم