{"id":652,"date":"2026-03-03T02:49:01","date_gmt":"2026-03-03T02:49:01","guid":{"rendered":"https:\/\/www.jccncmachining.com\/material\/\/"},"modified":"2026-03-03T02:49:01","modified_gmt":"2026-03-03T02:49:01","slug":"8620-%ea%b0%95","status":"publish","type":"material_model","link":"https:\/\/www.jccncmachining.com\/ko\/%ec%9e%ac%eb%a3%8c\/%ea%b0%95%ec%b2%a0\/8620-%ea%b0%95\/","title":{"rendered":"8620 \uac15"},"content":{"rendered":"<p><!-- Section: Machining Capabilities for 8620 Steel --><\/p>\n<div class=\"machining-capabilities\">\n<h3 style=\"font-size: 24px; font-weight: bold; margin-bottom: 15px;\">8620 \uac15\uc7ac \uac00\uacf5 \uc5ed\ub7c9<\/h3>\n<table style=\"width: 100%; border-collapse: collapse; margin-bottom: 30px;\" border=\"1\" cellspacing=\"0\" cellpadding=\"10\">\n<thead>\n<tr style=\"background-color: #f2f2f2;\">\n<th style=\"text-align: left; width: 25%;\">\uc5ed\ub7c9<\/th>\n<th style=\"text-align: left; width: 45%;\">\uae30\uc220 \uc124\uba85<\/th>\n<th style=\"text-align: left; width: 30%;\">Jucheng\uc758 \uac15\uc810<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td><strong>\uce68\ud0c4 \uc804 \uc120\uc0ad<\/strong><\/td>\n<td>\uce68\ud0c4 \ubc0f \ub2f4\uae08\uc9c8 \uacf5\uc815\uc744 \uc704\ud55c \uc815\ubc00 \uc5ec\uc720\ub97c \ub450\uace0 8620 \uc18c\uc7ac\ub97c \uadfc\uc811 \ud615\uc0c1\uc73c\ub85c \uac00\uacf5\ud569\ub2c8\ub2e4.<\/td>\n<td>\ub2f9\uc0ac\ub294 \uae30\uc5b4 \ube14\ub7ad\ud06c\uc6a9 \uace0\uc18d CNC \uc120\uc0ad\uc744 \uc81c\uacf5\ud558\uc5ec \uacbd\ud654 \uacf5\uc815 \uc804\uc5d0 \uc644\ubcbd\ud55c \ub3d9\uc2ec\ub3c4\ub97c \ubcf4\uc7a5\ud569\ub2c8\ub2e4.<\/td>\n<\/tr>\n<tr>\n<td><strong>\ubcf5\uc7a1\ud55c \uae30\uc5b4 \uc808\uc0ad<\/strong><\/td>\n<td>\uacf5\uad6c \uc218\uba85\uc744 \uadf9\ub300\ud654\ud558\uae30 \uc704\ud574 \uc5b4\ub2d0\ub9c1 \uc0c1\ud0dc\uc5d0\uc11c \ubcf5\uc7a1\ud55c \uae30\uc5b4 \uc774\uc640 \uc2a4\ud50c\ub77c\uc778\uc744 \ubc00\ub9c1 \ubc0f \ud638\ube59 \uac00\uacf5\ud569\ub2c8\ub2e4.<\/td>\n<td>\ub2f9\uc0ac\uc758 4\ucd95 \ubc0f 5\ucd95 \uc7a5\ube44\ub294 \uc5c4\uaca9\ud55c AGMA \ud488\uc9c8 \ud45c\uc900\uc744 \ucda9\uc871\ud558\ub294 \ubcf5\uc7a1\ud55c \uce58\ud615 \ud504\ub85c\ud30c\uc77c\uc744 \uc0dd\uc131\ud560 \uc218 \uc788\uc2b5\ub2c8\ub2e4.<\/td>\n<\/tr>\n<tr>\n<td><strong>\ud45c\uba74 \uacbd\ud654 \uad00\ub9ac<\/strong><\/td>\n<td>\ud2b9\uc815 \uacbd\ud654 \uae4a\uc774(\uc608: 0.5mm \u2013 1.5mm)\uc640 \ud45c\uba74 \uacbd\ub3c4\ub97c \ub2ec\uc131\ud558\uae30 \uc704\ud574 \uce68\ud0c4 \uacf5\uc815\uc744 \uad00\ub9ac\ud569\ub2c8\ub2e4.<\/td>\n<td>\ub2f9\uc0ac\ub294 \uad00\ub9ac\ud615 \uc5f4\ucc98\ub9ac\ub97c \uc81c\uacf5\ud558\uc5ec \uc2ec\ubd80\uc758 \uc778\uc131\uc744 \uc720\uc9c0\ud558\uba74\uc11c \ud45c\uba74 \uacbd\ub3c4 58-62 HRC\uc758 8620 \ubd80\ud488\uc744 \uacf5\uae09\ud569\ub2c8\ub2e4.<\/td>\n<\/tr>\n<tr>\n<td><strong>\uacbd\ud654 \ud6c4 \uc815\ubc00 \uc5f0\uc0ad<\/strong><\/td>\n<td>\uc5f4\ucc98\ub9ac\ub85c \uc778\ud55c \ubbf8\uc138\ud55c \ubcc0\ud615\uc744 \uad50\uc815\ud558\uae30 \uc704\ud574 \ubcf4\uc5b4, \uc800\ub110, \uce58\uc544\ub97c \uacbd\ud654 \ud6c4 \uc5f0\uc0ad\ud569\ub2c8\ub2e4.<\/td>\n<td>Jucheng\uc758 \uc815\ubc00 \uc5f0\uc0ad\uc740 \ucd5c\uc885 \uae30\uc5b4\uc640 \ud540\uc774 \uc870\uc6a9\ud558\uace0 \ub0b4\uad6c\uc131 \uc788\ub294 \uc791\ub3d9\uc744 \uc704\ud55c +\/- 0.005mm \uacf5\ucc28\ub97c \ucda9\uc871\ud558\ub3c4\ub85d \ubcf4\uc7a5\ud569\ub2c8\ub2e4.<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<\/div>\n<p><!-- Section: Fabrication Guidelines --><\/p>\n<div class=\"fabrication-guidelines\">\n<h3 style=\"font-size: 24px; font-weight: bold; margin-bottom: 15px;\">8620 \ud569\uae08\uac15 \uc81c\uc791 \uc9c0\uce68<\/h3>\n<p><strong>Carburizing Strategy:<\/strong><br \/>\n8620 is designed to be carburized. This adds carbon to the surface, allowing it to reach high hardness (60+ HRC) while the low carbon core remains ductile. <strong>\ud301:<\/strong> Ideal for parts subject to high shock and heavy surface wear.<\/p>\n<p><strong>\uae30\uacc4 \uac00\uacf5\uc131:<\/strong><br \/>\nIn its annealed state, 8620 has excellent machinability (approx. 65% of 1212). It shears cleanly and responds well to standard carbide tooling. <strong>\ud301:<\/strong> Maintain sharp tools to prevent surface tearing.<\/p>\n<p><strong>Distortion Control:<\/strong><br \/>\nQuenching can cause dimensional changes. <strong>\ud301:<\/strong> We recommend leaving 0.2mm to 0.4mm of grinding stock on critical diameters to be finished <em>\uc5f4\ucc98\ub9ac\ub97c \ud1b5\ud574 \uacbd\ud654\uc2dc\ud0a8<\/em> the hardening cycle.<\/p>\n<p><strong>\uc6a9\uc811\uc131:<\/strong><br \/>\n8620 can be welded easily in the annealed state using standard methods. However, welding after case-hardening is <strong>not recommended<\/strong> as it will destroy the surface properties.<\/p>\n<\/div>\n<p><!-- Section: Application Scenarios --><\/p>\n<div class=\"application-scenarios\">\n<h3 style=\"font-size: 24px; font-weight: bold; margin-bottom: 15px;\">\uc8fc\uc694 \uc751\uc6a9 \ubd84\uc57c<\/h3>\n<p><strong>Transmission &amp; Gearing<\/strong><br \/>\nDrive gears, pinions, splined shafts, and ring gears for automotive and heavy machinery industries.<\/p>\n<p><strong>\uc5d4\uc9c4 \uad6c\uc131\ud488<\/strong><br \/>\nCamshafts, piston pins, and tappets that require extreme surface wear resistance and high core toughness.<\/p>\n<p><strong>\uc0b0\uc5c5 \uae30\uacc4<\/strong><br \/>\n\ub192\uc740 \ucda9\uaca9\uacfc \ub9c8\ubaa8\ub97c \uacac\ub38c\uc57c \ud558\ub294 \uccb4\uacb0\uad6c, \ud540, \ubd80\uc2f1 \ubc0f \uc720\ub2c8\ubc84\uc124 \uc870\uc778\ud2b8.<\/p>\n<p><strong>\uc11d\uc720 \ubc0f \uac00\uc2a4 \uacf5\uad6c<\/strong><br \/>\n\uace0\uc555 \ub9c8\ucc30\uacfc \ucda9\uaca9 \ud558\uc911\uc5d0 \ub178\ucd9c\ub418\ub294 \uccb4\uc778 \ud540 \ubc0f \ub4dc\ub9b4 \ube44\ud2b8 \ubd80\ud488.<\/p>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>8620 Steel Machining Capabilities Capability Technical Description Jucheng Advantage Pre-Carburizing Turning Machining 8620 blanks to near-net shape with precise allowances for the carburizing and quenching process. We provide high-speed CNC turning for gear blanks, ensuring perfect concentricity before the hardening process. Complex Gear Cutting Milling and hobbing intricate gear teeth and splines in the annealed [&hellip;]<\/p>\n","protected":false},"featured_media":653,"template":"","meta":[],"class_list":["post-652","material_model","type-material_model","status-publish","has-post-thumbnail","hentry"],"_links":{"self":[{"href":"https:\/\/www.jccncmachining.com\/ko\/wp-json\/wp\/v2\/material_model\/652","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.jccncmachining.com\/ko\/wp-json\/wp\/v2\/material_model"}],"about":[{"href":"https:\/\/www.jccncmachining.com\/ko\/wp-json\/wp\/v2\/types\/material_model"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ko\/wp-json\/wp\/v2\/media\/653"}],"wp:attachment":[{"href":"https:\/\/www.jccncmachining.com\/ko\/wp-json\/wp\/v2\/media?parent=652"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}