{"id":1896,"date":"2026-08-08T17:47:06","date_gmt":"2026-08-08T09:47:06","guid":{"rendered":"https:\/\/www.jccncmachining.com\/?p=1896"},"modified":"2026-08-08T17:47:06","modified_gmt":"2026-08-08T09:47:06","slug":"machining-virgin-peek-solve-warping-tool-wear-precision-problems","status":"publish","type":"post","link":"https:\/\/www.jccncmachining.com\/ja\/blog\/machining-virgin-peek-solve-warping-tool-wear-precision-problems\/","title":{"rendered":"Machining Virgin PEEK: Solve Warping, Tool Wear &#038; Precision Problems"},"content":{"rendered":"<p>You have spent weeks designing a critical component\u2014a surgical instrument handle, an aerospace sensor housing, or a semiconductor wafer carrier. The material specification calls for Virgin PEEK, and you have sourced the expensive raw stock. Then the CNC machining begins, and within hours, the part warps, the surface finish looks like sandpaper, and the tool has worn beyond acceptable limits. This scenario plays out in machine shops around the world every day. The good news? It is entirely preventable. This guide walks through exactly how to machine Virgin PEEK successfully\u2014from understanding what makes this material extraordinary to mastering the speeds, feeds, and techniques that deliver consistent, precision results.<\/p>\n<p><img decoding=\"async\" width=\"1024\" height=\"768\" loading=\"lazy\" src=\"https:\/\/www.jccncmachining.com\/wp-content\/uploads\/2026\/08\/machining-virgin-peek.webp\" alt=\"Machining Virgin Peek\" class=\"alignnone size-full wp-image-1898\" \/>\n<hr srcset=\"https:\/\/www.jccncmachining.com\/wp-content\/uploads\/2026\/08\/machining-virgin-peek.webp 1024w, https:\/\/www.jccncmachining.com\/wp-content\/uploads\/2026\/08\/machining-virgin-peek-300x225.webp 300w, https:\/\/www.jccncmachining.com\/wp-content\/uploads\/2026\/08\/machining-virgin-peek-768x576.webp 768w\" sizes=\"(max-width: 1024px) 100vw, 1024px\" \/>\n<h2>What Makes Virgin PEEK Different from Every Other Plastic You Have Machined<\/h2>\n<p>Virgin PEEK\u2014polyetheretherketone in its pure, unfilled form\u2014sits at the top of the engineering thermoplastic pyramid. It is a semi-crystalline polymer with a continuous service temperature of 260\u00b0C (500\u00b0F) and a melting point around 343\u00b0C (649\u00b0F). The material offers outstanding chemical resistance, excellent wear properties, and remarkable dimensional stability. It resists hydrolysis, superheated steam, and a wide range of aggressive chemicals. In its virgin state, it provides the highest toughness and elongation of any PEEK grade, making it particularly suitable for medical implants, electrical insulators, and food processing components.<\/p>\n<p>But here is what the material datasheet does not tell you. Virgin PEEK behaves nothing like acetal, nylon, or other engineering plastics you may have machined. Its glass transition temperature of 143\u00b0C (289\u00b0F) means it stays rigid at temperatures where other polymers turn gummy. That is excellent for the finished part but creates real challenges on the shop floor. The material does not form the easy-to-break chips acetal produces\u2014chips can be stringy and may reweld to the surface if cutting speeds are too low.<\/p>\n<p>Perhaps the most critical factor that separates successful Virgin PEEK machining from costly failures is internal stress. Extruded PEEK rod and plate stock cools from the outside inward, locking compressive stress into the surface layer and tensile stress into the core. When you machine away material, you disrupt this stress balance. On a 100 mm diameter rod of unannealed stock, movement of 0.13 to 0.38 mm after rough machining is entirely possible. That is larger than many standard CNC tolerances. A straight cut can become a banana shape before your eyes.<\/p>\n<p>And then there is the cost consideration. A 50 mm diameter by 300 mm long rod of unfilled Virgin PEEK costs $150 to $300 depending on grade. Scrapping a part does not just cost cycle time\u2014it costs over $100 in raw material alone. This is why machining Virgin PEEK demands more planning, more process control, and more material-specific knowledge than any other engineering plastic.<\/p>\n<hr \/>\n<h2>The Five Core Challenges of Machining Virgin PEEK<\/h2>\n<p>Understanding the obstacles is the first step toward overcoming them. Based on extensive shop-floor experience and input from machining communities, these are the five challenges that consistently emerge when shops attempt to machine Virgin PEEK.<\/p>\n<h3>1. Heat Accumulation and Thermal Management<\/h3>\n<p>Virgin PEEK has low thermal conductivity. It does not dissipate heat the way metals do. Heat generated at the cutting interface stays concentrated, softening the polymer and causing smearing, melting, or deformation. This is the single most common cause of poor surface finish and dimensional drift in PEEK machining.<\/p>\n<p>Experienced machinists on forums frequently emphasize that managing heat is more important than any other parameter. One Reddit user noted, &#8220;Treat PEEK like it wants to melt if you look at it wrong\u2014because at the wrong speeds and feeds, it basically does.&#8221; The consensus among professionals is clear: keep the tool moving, avoid dwell time, and prioritize chip evacuation.<\/p>\n<h3>2. Residual Stress and Warping<\/h3>\n<p>As mentioned earlier, internal stress from the extrusion process is the hidden enemy of precision PEEK machining. Conventional shops that treat Virgin PEEK like any other plastic often discover warping only after the part is removed from the fixture\u2014at which point it is too late. Thin-walled components are especially vulnerable.<\/p>\n<p>One aerospace supplier reported that skipping the annealing step resulted in a 22% rejection rate due to ovality and distortion. After implementing proper stress-relief procedures, that rate dropped below 1%.<\/p>\n<h3>3. Tool Wear and Selection<\/h3>\n<p>Virgin PEEK may be unfilled, but it is still abrasive enough to dull standard carbide cutters rapidly. Dull tools increase cutting forces, generate more heat, and produce poor surface finishes. The machining community consistently recommends micro-grain solid carbide tools with polished flutes for unfilled PEEK. Silicon carbide tools are another good option.<\/p>\n<p>One shop supervisor put it this way: &#8220;If you hear your tool squeaking or see any discoloration on the chips, stop immediately. Your tool is already gone, and you are just burning money.&#8221;<\/p>\n<h3>4. Chip Control and Evacuation<\/h3>\n<p>Virgin PEEK produces stringy, continuous chips that can wrap around the tool or reweld to the workpiece surface. Poor chip evacuation leads to re-cutting, increased heat, and surface defects. Compressed air or vacuum systems are essential for clearing chips effectively.<\/p>\n<h3>5. Surface Finish and Burr Formation<\/h3>\n<p>PEEK tends to fray and burr, especially around small features, internal threads, or edges. For medical and aerospace components where debris is unacceptable, this creates significant quality challenges. High-speed micro-deburring tools, laser deburring, and single-flute reamers are common solutions.<\/p>\n<hr \/>\n<h2>Machining Virgin PEEK: Speeds, Feeds, and Parameters That Work<\/h2>\n<p>Getting the numbers right transforms Virgin PEEK machining from a gamble into a predictable process. The following parameters represent industry consensus based on extensive testing and real-world production experience.<\/p>\n<h3>Recommended Cutting Parameters for Virgin PEEK<\/h3>\n<table>\n<thead>\n<tr>\n<th><strong>Operation<\/strong><\/th>\n<th><strong>Cutting Speed (m\/min)<\/strong><\/th>\n<th><strong>Feed Rate<\/strong><\/th>\n<th><strong>Depth of Cut<\/strong><\/th>\n<th><strong>Tool Recommendation<\/strong><\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td><strong>Milling &#8211; Roughing<\/strong><\/td>\n<td>150 &#8211; 300<\/td>\n<td>0.05 &#8211; 0.15 mm\/tooth<\/td>\n<td>0.5 &#8211; 1.0 mm axial<\/td>\n<td>Micro-grain carbide, 2-3 flute<\/td>\n<\/tr>\n<tr>\n<td><strong>Milling &#8211; Finishing<\/strong><\/td>\n<td>200 &#8211; 400<\/td>\n<td>0.05 &#8211; 0.10 mm\/tooth<\/td>\n<td>0.1 &#8211; 0.3 mm<\/td>\n<td>Sharp carbide, polished flutes<\/td>\n<\/tr>\n<tr>\n<td><strong>Turning<\/strong><\/td>\n<td>200 &#8211; 400<\/td>\n<td>0.10 &#8211; 0.30 mm\/rev<\/td>\n<td>0.5 &#8211; 2.0 mm<\/td>\n<td>Carbide with positive rake<\/td>\n<\/tr>\n<tr>\n<td><strong>Drilling<\/strong><\/td>\n<td>50 &#8211; 100<\/td>\n<td>0.05 &#8211; 0.15 mm\/rev<\/td>\n<td>N\/A<\/td>\n<td>Sharp HSS or carbide, frequent retract<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>Source: Industry machining guides and parameter databases<\/p>\n<p>The sweet spot for unfilled Virgin PEEK milling is generally 300\u2013600 SFM (91\u2013183 m\/min)\u2014roughly twice the speed used for acetal. For a 6 mm two-flute carbide cutter at 180 m\/min, this converts to approximately 9,550 RPM with a feed of about 764 mm\/min at 0.04 mm\/tooth.<\/p>\n<p>Climb milling is strongly preferred over conventional milling. It produces lower cutting forces, better surface finish, and less heat input. For threading, single-point threading on a lathe produces the most accurate PEEK threads.<\/p>\n<h3>Cooling Strategies That Protect Both Tool and Part<\/h3>\n<p>The cooling approach depends on the application. For industrial-grade Virgin PEEK, flood coolant with a water-soluble or light oil-based coolant works well. High-pressure nozzles should target the tool-workpiece interface directly.<\/p>\n<p>For medical-grade Virgin PEEK, however, oil-based coolants must be avoided to maintain biocompatibility. Compressed air at 5\u20137 bar or deionized water is the standard approach. Keep the air nozzle moving to avoid local chilling, which can induce brittleness.<\/p>\n<p>Some shops report success with minimum quantity lubrication (MQL) for less aggressive operations. Flood coolant is generally not recommended for PEEK, as thermal shock from cold coolant on a warm part can induce micro-cracks.<\/p>\n<hr \/>\n<h2>The Annealing Protocol: Your Insurance Policy Against Warping<\/h2>\n<p>If there is one step that separates professionals from amateurs in Virgin PEEK machining, it is annealing. This thermal treatment relieves internal stresses, increases crystallinity to 35\u201340%, and stabilizes the material structure. Skipping it risks dimensional drift and part rejection during final inspection.<\/p>\n<p>Annealing raw Virgin PEEK stock before machining is standard practice. The process involves:<\/p>\n<ul>\n<li><strong>Ramp:<\/strong> Heat the material gradually to 200\u2013220\u00b0C in a controlled oven<\/li>\n<li><strong>Soak:<\/strong> Maintain temperature for 1\u20132 hours, with approximately 30 minutes per 10 mm of material thickness<\/li>\n<li><strong>Slow Cool:<\/strong> Turn off the oven and allow the material to cool to room temperature over several hours\u2014never remove parts while hot<\/li>\n<\/ul>\n<p>For complex parts with heavy material removal, an intermediate anneal after rough machining and before finishing is highly recommended. This allows stresses released during roughing to stabilize before the final precision cuts.<\/p>\n<p>One Jucheng Precision engineer describes the annealing process as the &#8220;secret that unlocks the full potential of Virgin PEEK&#8221;. The material arrives with internal stresses that are invisible but very real. Cutting away the stressed outer layers without first relieving those stresses causes the material to move, warp, or bend during machining.<\/p>\n<hr \/>\n<h2>Where Virgin PEEK Components Make the Difference<\/h2>\n<p>Virgin PEEK&#8217;s unique combination of properties\u2014biocompatibility, chemical resistance, thermal stability, and mechanical strength\u2014makes it the material of choice across multiple demanding industries.<\/p>\n<h3>Medical and Healthcare Applications<\/h3>\n<p>Virgin PEEK&#8217;s biocompatibility and radiolucency (transparency to X-rays) have revolutionized medical device manufacturing. It is used for spinal fusion cages, cranial implants, surgical instruments, and endoscope components. The material can be sterilized repeatedly via steam autoclave, gamma radiation, or ethylene oxide without degradation.<\/p>\n<p>Medical-grade Virgin PEEK must meet ISO 10993 and USP Class VI standards. Machining these parts requires exceptionally clean environments and processes that maintain material purity.<\/p>\n<h3>Aerospace and Defense<\/h3>\n<p>In aerospace applications, Virgin PEEK replaces metal in mission-critical but non-structural components: clips, spacers, insulators, and fluid connectors. The material offers a strength-to-weight ratio comparable to aluminum at half the weight. Its flame retardancy (UL 94 V-0 rating) and low smoke emission make it suitable for aircraft interior applications.<\/p>\n<h3>Semiconductor and Electronics<\/h3>\n<p>Virgin PEEK&#8217;s electrical insulation properties, chemical resistance, and thermal stability make it ideal for semiconductor wafer carriers, electrical insulators, and connector housings. The material maintains its properties in cleanroom environments and resists the aggressive chemicals used in semiconductor manufacturing.<\/p>\n<h3>Oil and Gas<\/h3>\n<p>Downhole drilling environments demand materials that withstand extreme temperatures, pressures, and chemical exposure. Virgin PEEK components\u2014seals, backup rings, and electrical connectors\u2014perform reliably where other plastics fail.<\/p>\n<hr \/>\n<h2>Achievable Tolerances and Quality Standards<\/h2>\n<p>With proper technique and process control, Virgin PEEK can hold surprisingly tight tolerances. For most applications, standard machining achieves tolerances of \u00b10.05 mm (\u00b10.002\u2033). For high-precision components under controlled conditions, tolerances as tight as \u00b10.012 mm (\u00b10.0005\u2033) are achievable.<\/p>\n<p>Surface finish requirements vary by application. Medical and aerospace components often specify Ra values below 0.8 \u03bcm. Achieving this requires sharp tools, fine finishing passes, and proper chip evacuation.<\/p>\n<p>Quality verification typically involves coordinate measuring machine (CMM) inspection. Advanced shops like Jucheng Precision use Zeiss CMM metrology to verify every critical dimension.<\/p>\n<hr \/>\n<h2>Why Partner with a Specialist for Virgin PEEK Machining<\/h2>\n<p>Virgin PEEK machining is not a process that can be learned overnight. The material demands specific knowledge, disciplined processes, and specialized equipment. This is where partnering with an experienced CNC machining provider makes the difference between success and costly failure.<\/p>\n<p><strong>Jucheng Precision<\/strong> has extensive expertise in Virgin PEEK CNC machining services, processing premium PEEK grades from standard virgin material to specialized implantable grades. The company operates a high-precision manufacturing floor certified to <strong>AS9100<\/strong> (aerospace), <strong>ISO 13485<\/strong> (medical devices), <strong>IATF 16949<\/strong> (automotive), and <strong>ISO 9001<\/strong> quality standards.<\/p>\n<p>What sets Jucheng apart in Virgin PEEK machining is the systematic approach to thermal management. The company has elevated annealing to a science, ensuring every component is dimensionally stable and structurally &#8220;dead&#8221;\u2014meaning no residual stress remains to cause future warping. Their facility includes dedicated clean-room 5-axis CNC workstations managed by certified technicians.<\/p>\n<p>The company&#8217;s knowledge base includes detailed guides on PEEK annealing, high-temperature stabilization, tool selection, and achieving low-volume precision for medical and aerospace prototypes. With over 150 CNC machines and advanced metrology equipment, Jucheng delivers components that meet the most demanding specifications.<\/p>\n<p>For design engineers and procurement professionals, the value proposition is clear: Virgin PEEK is too expensive and too demanding to trust to a generalist shop. Working with a specialist who understands the material&#8217;s &#8220;personality&#8221; and has the process controls to match reduces risk, improves quality, and ultimately lowers total cost.<\/p>\n<hr \/>\n<h2>Frequently Asked Questions About Machining Virgin PEEK<\/h2>\n<h3>1. What is the difference between Virgin PEEK and filled PEEK grades?<\/h3>\n<p>Virgin PEEK is the pure, unfilled polymer. It offers the highest toughness, elongation, and chemical resistance of all PEEK grades. Glass-filled PEEK (GF30) adds glass fibers for increased stiffness and creep resistance but is more abrasive to tools. Carbon-filled PEEK (CF30) provides the highest strength, stiffness, and wear resistance. Virgin PEEK is generally easier to machine than reinforced variants and is preferred for medical, food contact, and electrical insulation applications.<\/p>\n<h3>2. Can Virgin PEEK be machined on standard CNC equipment?<\/h3>\n<p>Yes, Virgin PEEK can be machined using standard metalworking CNC equipment. However, success depends on using the right tools, parameters, and processes. Standard metal-cutting parameters will not work\u2014PEEK requires specific speeds, feeds, and cooling strategies. Shops without PEEK-specific experience often struggle with warping, poor surface finish, and excessive tool wear.<\/p>\n<h3>3. Why does Virgin PEEK warp during machining?<\/h3>\n<p>Warping occurs because extruded PEEK stock contains internal stresses from the cooling process. When you machine away material, you release these stresses unevenly, causing the part to deform. The solution is annealing\u2014heating the material to 200\u2013220\u00b0C before machining to relieve internal stresses. Intermediate annealing after roughing is also recommended for complex parts.<\/p>\n<h3>4. What tools work best for machining Virgin PEEK?<\/h3>\n<p>Micro-grain solid carbide tools with polished flutes provide the best combination of sharpness, edge retention, and cost for Virgin PEEK. Silicon carbide tools are another good option. Tools should have positive rake angles and sharp cutting edges. For filled PEEK grades, polycrystalline diamond (PCD) or diamond-coated tools may be necessary.<\/p>\n<h3>5. What are the recommended speeds and feeds for Virgin PEEK milling?<\/h3>\n<p>For milling Virgin PEEK, recommended cutting speeds range from 150\u2013300 m\/min for roughing and 200\u2013400 m\/min for finishing. Feed rates typically range from 0.05\u20130.15 mm\/tooth. The sweet spot for unfilled PEEK is 300\u2013600 SFM (91\u2013183 m\/min)\u2014roughly twice the speed used for acetal. Climb milling is preferred over conventional milling.<\/p>\n<h3>6. What cooling method should I use for Virgin PEEK?<\/h3>\n<p>For industrial-grade Virgin PEEK, flood coolant with water-soluble or light oil-based coolant works well. For medical-grade PEEK, use compressed air at 5\u20137 bar or deionized water to maintain biocompatibility. Flood coolant is generally not recommended as thermal shock can induce micro-cracks. The primary goal is efficient chip removal.<\/p>\n<h3>7. What tolerances can Virgin PEEK achieve?<\/h3>\n<p>Standard machining achieves tolerances of \u00b10.05 mm (\u00b10.002\u2033) for most applications. Under controlled conditions with proper techniques, tolerances as tight as \u00b10.012 mm (\u00b10.0005\u2033) are possible. Achieving these tolerances requires annealing, sharp tools, proper cooling, and stable environmental conditions.<\/p>\n<h3>8. Is Virgin PEEK suitable for medical implants?<\/h3>\n<p>Yes, specific Virgin PEEK grades meet ISO 10993 and USP Class VI standards for biocompatibility. Medical-grade Virgin PEEK is used for spinal fusion cages, cranial implants, and surgical instruments. It is radiolucent (transparent to X-rays), allowing bone visibility in imaging. Machining medical-grade PEEK requires clean environments and processes that maintain material purity.<\/p>\n<h3>9. Why is Virgin PEEK so expensive?<\/h3>\n<p>Virgin PEEK is a high-performance engineering thermoplastic manufactured through complex polymerization processes. A 50 mm diameter by 300 mm long rod costs $150\u2013300. The material&#8217;s exceptional properties\u2014thermal stability to 260\u00b0C, chemical resistance, biocompatibility, and mechanical strength\u2014justify the cost for mission-critical applications. Scrapping a part during machining adds significant expense, which is why proper process control is essential.<\/p>\n<h3>10. How does Virgin PEEK compare to metal for component manufacturing?<\/h3>\n<p>Virgin PEEK offers a strength-to-weight ratio comparable to some aluminum alloys at 50% lower weight. It provides chemical resistance that metals cannot match, resists corrosion, and is radiolucent for medical imaging. PEEK components can be machined to tight tolerances without the need for costly mold tooling. For applications requiring weight reduction, chemical resistance, or biocompatibility, Virgin PEEK often outperforms metal alternatives.<\/p>\n<hr \/>\n<h2>Putting It All Together: Your Virgin PEEK Machining Action Plan<\/h2>\n<p>Successful Virgin PEEK machining comes down to following a disciplined process. Here is a practical checklist based on industry best practices and shop-floor experience:<\/p>\n<ol>\n<li><strong>Start with annealed stock<\/strong>\u2014Never machine raw PEEK without first relieving internal stresses through controlled annealing<\/li>\n<li><strong>Select the right tools<\/strong>\u2014Micro-grain carbide with polished flutes for unfilled PEEK<\/li>\n<li><strong>Optimize speeds and feeds<\/strong>\u2014300\u2013600 SFM for milling, with appropriate feed rates<\/li>\n<li><strong>Use climb milling<\/strong>\u2014Reduces cutting forces and heat generation<\/li>\n<li><strong>Manage heat aggressively<\/strong>\u2014Proper cooling and chip evacuation are non-negotiable<\/li>\n<li><strong>Take light cuts<\/strong>\u20140.5\u20131.0 mm for roughing, 0.1\u20130.3 mm for finishing<\/li>\n<li><strong>Avoid tool dwell<\/strong>\u2014Keep the tool moving to prevent localized heating<\/li>\n<li><strong>Consider intermediate annealing<\/strong>\u2014For complex parts with heavy material removal<\/li>\n<li><strong>Inspect regularly<\/strong>\u2014Check tool edges and part dimensions throughout the run<\/li>\n<li><strong>Work with specialists<\/strong>\u2014Partner with a shop that understands PEEK&#8217;s unique requirements<\/li>\n<\/ol>\n<p>Virgin PEEK machining is challenging, but it is not mysterious. The material behaves predictably when you understand its properties and respect its limitations. With the right knowledge, tools, and processes, you can consistently produce high-quality Virgin PEEK components that meet the most demanding application requirements.<\/p>\n<p>Whether you are designing medical implants, aerospace components, or semiconductor equipment, the key to success lies in treating Virgin PEEK with the respect it deserves\u2014and partnering with machining experts who have mastered the art and science of working with this extraordinary material.<\/p>\n<hr \/>\n<p><strong>Ready to discuss your Virgin PEEK machining project?<\/strong> Jucheng Precision&#8217;s team of PEEK machining specialists is available to review your design, recommend optimal grades and processes, and deliver precision components that meet your exact specifications. <a href=\"https:\/\/www.jccncmachining.com\/ja\/\" rel=\"nofollow\">Contact Jucheng Precision today<\/a> to start your project with a partner who understands what it takes to machine Virgin PEEK right the first time.<\/p>","protected":false},"excerpt":{"rendered":"<p>You have spent weeks designing a critical component\u2014a surgical instrument handle, an aerospace sensor housing, or a semiconductor wafer carrier. The material specification calls for Virgin PEEK, and you have sourced the expensive raw stock. Then the CNC machining begins, and within hours, the part warps, the surface finish looks like sandpaper, and the tool has worn beyond acceptable limits. This scenario plays out in machine shops around the world every day. The good news? It is entirely preventable. This guide walks through exactly how to machine Virgin PEEK successfully\u2014from understanding what makes this material extraordinary to mastering the speeds, feeds, and techniques that deliver consistent, precision results. What Makes [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":1898,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1],"tags":[],"class_list":["post-1896","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-blog"],"_links":{"self":[{"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/posts\/1896","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/comments?post=1896"}],"version-history":[{"count":2,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/posts\/1896\/revisions"}],"predecessor-version":[{"id":1899,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/posts\/1896\/revisions\/1899"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/media\/1898"}],"wp:attachment":[{"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/media?parent=1896"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/categories?post=1896"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.jccncmachining.com\/ja\/wp-json\/wp\/v2\/tags?post=1896"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}